Seven measures to reduce defects in mold processing

Release time:2021-08-23

In order to improve the performance of the mold, many manufacturers will process the mold properly. Mold processing refers to the processing of forming and punching tools. In addition, it also includes cutting die and die-cutting die. However, in many cases, the mold is processed. It will also reflect processing defects, resulting in the decline of mold performance. How to establish mold processing defects? The following seven measures can accumulate mold processing defects.


1. Reasonable selection and dressing of grinding wheel


White corundum grinding wheel is better. Its performance is hard and brittle, and it is easy to produce new cutting edges. Therefore, the cutting force is small and the grinding heat is small. Select medium particle size, such as 46 ~ 60 mesh. The hardness of the grinding wheel is medium soft and medium soft (ZR1, Zr2 and R1, R2), that is, coarse-grained, low hardness grinding wheel, good self excitation can reduce the cutting heat.


It is very important to choose a suitable grinding wheel for fine grinding. GD single crystal corundum grinding wheel is more suitable for high vanadium and high molybdenum conditions of die steel. When machining cemented carbide and materials with high quenching hardness, organic bond diamond is preferred. The self grinding performance of grinding wheel and organic bond grinding wheel is good, and the roughness of grinding workpiece can reach Ra0.2 μ m。 In recent years, with the application of new materials, CBN (cubic boron nitride) grinding wheels have shown good machining results. The effect of finish machining on CNC forming grinder, coordinate grinder and CNC Internal and external grinder is better than that of other types of grinding wheels.


In the grinding process, attention should be paid to timely dressing the grinding wheel to keep it sharp. After passivation, the grinding wheel will slip and squeeze on the surface of the workpiece, causing burns on the surface of the workpiece and reducing its strength.


2. Rational use of cooling lubricants


Play the three functions of cooling, flushing and lubrication, keep the cooling and lubrication clean, control the grinding heat within the allowable range, and prevent the thermal deformation of the workpiece. Improve the cooling conditions during grinding, such as using oil immersed grinding wheel or internally cooled grinding wheel. When the cutting fluid is introduced into the center of the grinding wheel, the cutting fluid can directly enter the grinding area, which has an effective cooling effect and prevents the workpiece surface from being burned.


3. Try to reduce the quenching stress after heat treatment


Due to the effect of quenching stress and grinding force, the phase transformation of network carbonized structure is easy to cause workpiece cracks. For high-precision dies, in order to eliminate grinding residual stress, low-temperature aging treatment should be carried out after grinding to improve toughness.


4. Eliminate grinding stress


The mold can also be immersed in a salt bath at 260 ~ 315 ℃ for 1.5 minutes, and then cooled in oil at 30 ℃, which can reduce the hardness by 1hrc and the residual stress by 40% - 65%.


5. Constant temperature grinding


For precision grinding of precision dies with dimensional tolerance within 0.01mm, attention should be paid to the influence of ambient temperature, and constant temperature grinding is required. The calculation shows that for a 300mm long steel, when the temperature difference is 3 ℃, the material will have 10.8 μ Change about M (10.8=1.2 × three × 3. The deformation per 100mm is 1.2 μ M/ ℃), and each finishing process needs to consider the influence of this factor.


6. Electrolytic grinding processing


Improve mold manufacturing accuracy and surface quality. During electrolytic grinding, the grinding wheel scrapes off the oxide film: instead of grinding metal, the grinding force is small, the grinding heat is small, and there will be no grinding burrs, cracks, burns, etc. the surface roughness can generally be better than ra0.16 μ m; In addition, the wear of grinding wheel is small, such as the grinding of cemented carbide. The wear amount of silicon carbide grinding wheel is about 400% - 600% of the weight of cemented carbide being ground. When electrolytic grinding is used, the wear of grinding wheel can only remove 50% - 100% of cemented carbide.


7. Reasonable selection of grinding amount


Fine grinding mode is adopted, with small radial feed and uniform fine grinding. If the radial feed rate and the speed of the grinding wheel are properly reduced and the axial feed rate is increased, the contact area between the grinding wheel and the workpiece can be reduced, the heat dissipation conditions can be improved and the temperature of the workpiece can be increased. The surface can be effectively controlled.

Copyright: Shenzhen Zhongyuan Plastic Co., Ltd. | mold processing customized manufacturer. If you want to know the processing price of the factory, how much is it, and which is good, please contact us Yue ICP Bei No. 17060480
主站蜘蛛池模板: 精品国产一区二区三区久久久狼 | 国产精品无码一区二区三区电影| 国产小屁孩cao大人| 国产熟人av一二三区| 免费人成网站视频在线观看国内| 久久综合九色综合欧美狠狠| 国产香港明星裸体xxxx视频| 亚洲欧美日韩国产综合一区二区| 国产卡一卡二卡三免费入口| 亚洲国产精品无码久久久秋霞2| 中文字幕人成无码人妻综合社区 | 在办公室被c到呻吟的动态图 | 狠狠精品久久久无码中文字幕| 最近免费中文字幕大全高清10| 影视先锋av资源噜噜| 人体内射精一区二区三区| 亚洲伊人成无码综合网| 男受被做哭激烈娇喘gv视频| 亚洲精品成人a在线观看| 亚洲av福利院在线观看| www国产精品内射熟女| 国产精品jizz在线观看老狼| 色爱情人网站| 婷婷综合久久中文字幕蜜桃三电影| 国产白嫩漂亮美女在线观看| 亚洲精品国产精品乱码不99| 本道天堂成在人线av无码免费| 自拍偷自拍亚洲精品播放 | 色www永久免费视频| 国产午夜精品一区二区三区漫画| 寂寞骚妇被后入式爆草抓爆| 中文字幕制服丝袜第57页| 99久热re在线精品99 6热视频| 8天堂资源在线| 久久亚洲精品无码gv| 97久久综合亚洲色hezyo| 国产动作大片中文字幕| 蜜臀av无码精品人妻色欲| 奇米在线7777在线精品| 久久亚洲精品情侣| 亚洲精品92内射|